Best Glue for PETG 3D Prints: Hands-On Adhesive Test Results
We had a cracked PETG drone arm on the bench, three different glues on the shelf, and an afternoon to find out which one would actually hold. The answer turned out to be not the one on the tube that said "bonds all plastics."
If you've searched for the best glue for PETG 3D prints and ended up with conflicting forum posts, this is the test we wished existed. We printed identical coupons, bonded them with every adhesive we had, and pulled them apart on a shop-built rig. Numbers, failure modes, and the one surface prep step that doubled our strongest result.
No sponsored picks. Just what broke, what held, and what we'd reach for next time.
Why PETG Is Harder to Glue Than PLA or ABS
PETG is glycol-modified polyethylene terephthalate. The glycol is there to stop the polymer crystallizing during extrusion, which is what makes it tough, clear, and layer-adhesion friendly. That same chemistry is why glue struggles.
PLA is reactive enough that cyanoacrylate bites into it cleanly. ABS dissolves in acetone, so you can smear on a slurry and watch it weld to itself. PETG does neither. It has a slick, low-surface-energy face that most adhesives bead on rather than wet out.
The Prusa PETG material guide notes that PETG prints are chemically closer to drink-bottle plastic than to engineering ABS, which is exactly why solvents that chew through ABS leave PETG shiny and untouched. Any glue that works on PETG is either biting mechanically into the surface texture, reacting with the glycol fraction, or being carried in by a solvent strong enough to actually swell the polymer.
That gives you three honest options: cyanoacrylate for speed, epoxy for strength, or a purpose-built PETG adhesive. Everything else in the drawer is a coin flip, and the All3DP PETG adhesion overview lines up with what we measured on the bench.
How We Tested: Print Settings, Bond Area, and Stress Rig
We printed 48 coupons on our shop's enclosed FDM machine using PETG in black, 0.2 mm layer height, 4 walls, 40% gyroid infill. Each coupon was 60 mm × 20 mm × 4 mm with a flat lap-joint face. Same spool, same bed, same day.
Bond area was fixed at 20 mm × 20 mm per joint, measured with calipers before the adhesive went on. Half the samples got no prep. The other half got a 10-second scuff with fresh 220-grit, isopropyl wipe, and a 60-second flash-off.
Cure happened on a shelf at 21 °C and 38% RH. We held each adhesive to its own manufacturer-stated full cure, not just handling time. Five-minute epoxy sat 24 hours. Standard CA sat four hours.
The test rig is a scrap-steel lap-shear jig pulled with a hydraulic bottle jack running against a 500 kg load cell we had calibrated for a different project. Three pulls per adhesive per prep state, mean reported below. Failure modes were photographed and tagged as adhesive (clean release), cohesive (glue tore internally), or substrate (PETG itself fractured).
The useful signal isn't the raw kilonewtons. It's which combinations failed brittle, which failed ductile, and which pulled the print apart before the joint moved.
Cyanoacrylate (CA / Super Glue) on PETG: Fast but Brittle
CA sets fast on PETG, faster than we expected. A thin layer of standard Loctite 401 kicked in about 40 seconds with no accelerator and reached handling strength in under two minutes. Gel formulas were slower, around 90 seconds, but filled small print-line gaps better.
Strength is where CA earns its reputation for disappointing people. Unprepped coupons held 1.8 MPa average shear. With a 220-grit scuff that climbed to 2.4 MPa, a real but modest gain. Every single CA joint failed adhesive, meaning the glue let go cleanly from the PETG face without tearing a fiber.
Accelerator cut cure time to under 10 seconds but dropped strength another 20%. The flash cure doesn't give the adhesive time to wet the surface before it locks up, so you get a brittle crust sitting on top of the plastic rather than keyed into it.
Where CA is the right call: cosmetic repairs, tacking parts in place before an epoxy pour, miniatures, display pieces, anything where the joint won't see shock or shear. It's also the only option in our test that cured fast enough to hold a part in orientation while you got on with something else.
Where it fails: anything functional. We snapped a CA'd drone-arm repair with a gentle desk-corner knock. The joint didn't yield, it shattered. If the part will see load, impact, or vibration, skip to the next section.
Two-Part Epoxy on PETG: The Strength Winner
Epoxy won. Not close. Loctite 5-minute at 24 hours of cure hit 6.1 MPa on scuffed coupons, more than triple the best CA result. JB Weld 24-hour epoxy pushed to 7.4 MPa and about half the samples failed substrate, meaning the PETG itself tore before the bondline did.
Surface prep is not optional with epoxy on PETG. Unprepped samples averaged 3.2 MPa, respectable but half of what the scuffed samples gave us. The 220-grit bite lets the resin key into surface topography that PETG's glossy face otherwise denies it.
Failure modes shifted with cure time too. The 5-minute epoxy failed cohesive, tearing apart inside the glue layer rather than at the plastic. That tells us the resin itself was the weak link, not the bond interface. The longer-cure epoxy didn't have that ceiling.
Mix ratio matters more than people say. Off-ratio epoxy, especially the double-syringe kind where one side plunges slower than the other, cures soft and chalky. Weigh it on a $15 jeweler's scale if the joint is structural. We saw 30% strength loss in a batch where the hardener was visibly leaner than the resin.
Fillers help gap-bridging. Microballoons or even a pinch of printer dust thicken the mix without hurting strength, useful because 3D-printed surfaces are rarely dead flat. Keep the fill under 20% by volume or you start robbing resin from the interface.
Solvent Welding PETG: What Actually Works
PETG is where the "just use ABS slurry" advice falls apart. Acetone does nothing. MEK does almost nothing. We swabbed both on a test coupon, let them sit two minutes, and the surface was unchanged under a loupe.
Dichloromethane (DCM, methylene chloride) is the one that works. It's what industrial PET plumbing uses. A thin bead on both faces, pressed together under light clamp pressure, gave us a weld that hit 5.8 MPa and failed substrate on two of three pulls.
The catch is real. DCM is a suspected carcinogen, boils at 40 °C, and is restricted or banned for consumer paint-stripper use in several countries. It requires gloves rated for halogenated solvents (nitrile dissolves), outdoor use or a fume hood, and a respirator with organic-vapor cartridges. You cannot buy it at a hardware store in the US anymore for general consumer use.
Tetrahydrofuran (THF) also works and is slightly less nasty. Still not something to open in your kitchen. For the overwhelming majority of makers, solvent welding PETG is not the practical answer, even though chemically it is a strong one.
If you are set up for it and your part is a sealed pressure vessel or something else where a continuous homogeneous joint matters, DCM will give you the cleanest result on this list. For everyone else, epoxy is 90% of the strength without the respirator.
3D Gloop and Purpose-Built PETG Adhesives
3D Gloop sells a PETG-specific formula that behaves like a thick solvent cement. It smells like a milder cousin of MEK, flows like honey, and grabs in about 30 seconds.
We measured 5.4 MPa on scuffed PETG coupons and 4.6 MPa unprepped. That puts it comfortably above CA, within striking distance of 5-minute epoxy, and well short of 24-hour epoxy. Failure was mostly cohesive, inside the glue line, which is the giveaway that it's working as a solvent-plus-polymer filler rather than a pure weld.
The real win is workflow. One bottle, no mixing, no ratio errors, no 24-hour wait. For multi-part PETG assemblies where you're bonding a dozen seams and don't want to live at the epoxy bench for a weekend, 3D Gloop is the sensible pick.
Where it loses to epoxy: the joint stays slightly elastic, which is great for drop resistance but costs you ultimate strength. If the part is a motor mount or anything that sees cyclic load, run the epoxy.
Our Verdict: Best Glue for PETG 3D Prints by Use Case
The right answer depends on what the joint has to do, not which adhesive is strongest in isolation. Here's how we'd sort it on a Monday morning with a broken print in hand.
| Adhesive | Shear Strength (scuffed) | Full Cure | Failure Mode | Best Use |
|---|---|---|---|---|
| Cyanoacrylate (standard) | 2.4 MPa | 4 h | Adhesive, brittle | Cosmetic, tacking |
| 5-minute epoxy | 6.1 MPa | 24 h | Cohesive | General structural |
| 24-hour epoxy (JB Weld) | 7.4 MPa | 24 h | Substrate | Load-bearing, final |
| DCM solvent weld | 5.8 MPa | 10 min | Substrate | Sealed joints (PPE only) |
| 3D Gloop PETG | 5.4 MPa | 2 h | Cohesive | Multi-part assembly |
Cosmetic chip or display piece: CA, gel formula, no accelerator. Thirty seconds of pressure and you're done.
Functional load-bearing joint: 24-hour epoxy on a 220-grit scuff. Weigh the mix. Clamp light, not hard, to keep a wet glue line.
Multi-part assembly you want done today: 3D Gloop. Buy the actual PETG formula, not the generic one.
Field repair with no shop access: whatever CA is in the glovebox and an understanding that it's a bridge, not a fix.
FAQ
Does super glue work on PETG?
Yes, cyanoacrylate bonds PETG quickly, but the joint is brittle under stress. Standard thin CA kicks in under a minute on bare PETG and reaches handling strength in two. It's fine for cosmetic parts, miniatures, and tacking joints before a stronger glue sets. For anything load-bearing, use epoxy or 3D Gloop instead.
Can you solvent weld PETG like ABS?
Not with the usual shop solvents. PETG resists acetone and MEK, which readily dissolve ABS. Dichloromethane does work and gives substrate-level strength, but it is a restricted, hazardous solvent that needs proper gloves and ventilation. For most makers, epoxy or a PETG-specific adhesive like 3D Gloop is the practical choice.
What's the strongest glue for PETG prints?
Two-part epoxy with a lightly sanded bond surface produced the highest shear strength in our tests, roughly three times cyanoacrylate. A 24-hour cure epoxy like JB Weld reached 7.4 MPa and often tore the PETG itself before the bondline failed. Five-minute epoxy is a usable second if you need the part today.
Do I need to sand PETG before gluing?
For load-bearing joints, yes. A quick scuff with 220-grit roughly doubled epoxy shear strength in our test by giving the adhesive mechanical bite on PETG's slick, low-surface-energy face. Wipe with isopropyl after sanding to remove dust and let it flash off for a minute before applying glue.
Will 3D Gloop work on PETG?
3D Gloop makes a PETG-specific formula that outperforms generic CA and rivals 5-minute epoxy on bond strength. The convenience advantage is big: one bottle, no mixing, no ratio errors, and handling strength in about 30 seconds. It falls short of a 24-hour epoxy for ultimate load-bearing joints, but it's the right pick for multi-part assemblies.
Closing
Buy one tube of good epoxy, one bottle of CA, and if you print PETG often, a bottle of a PETG-specific adhesive. That covers 95% of what comes off the printer broken or in pieces. Keep 220-grit near the glue shelf so the surface prep step isn't a reason to skip it.
If you're deciding whether PETG is even the right material for a part you're about to print, our write-up on PLA filament vs PETG: which spool for your project walks through the trade-offs before you load the spool.